A round bar, 10 mm diameter and 50 mm gauge length, is pulled to fracture. Choose a reference material, or enter your student ID to get your own unknown specimen. The same ID always gives the same specimen and the same scatter, so your results can be checked. Download the CSV and do the analysis yourself before you use Part 2.
- Max load
- –
- UTS (eng.)
- –
- Uniform elong.
- –
- Elong. at fracture
- –
Load scatter is about ±0.2% of the maximum load and the extensometer reads to about ±2 µm, as in a real test. The shape after necking is illustrative only: once the neck forms, strain is no longer uniform and the gauge-length data cannot be turned into true stress and strain.
Between yield and the maximum load, many metals follow σ = Kεⁿ. On log–log axes that is a straight line of slope n, crossing ε = 1 at σ = K. Which points you include changes the answer. Choose the strain window, decide whether to remove the elastic strain, and watch n move. Then enter the values you found yourself and check them.
- Fitted n
- –
- Fitted K
- –
- R²
- –
- Points used
- –
Grey points are outside the window or past the maximum load. The line is the least-squares fit of ln σ on ln ε over the coloured points.
Check your own analysis
Work from the CSV in a spreadsheet or Python, not from this page. Enter your K and n. The lab says whether they agree with the specimen within ±6% for K and ±0.02 for n, without giving the answer away.
Necking check
For σ = Kεⁿ the maximum load comes at a true strain ε = n (Considère condition, reference 3), so the engineering UTS should be K·nⁿ·e⁻ⁿ. Compare this with the UTS you measured.
- UTS from fit
- –
- UTS measured
- –
- Difference
- –
A solid cylinder is upset between flat dies with sliding friction. The slab method gives the average die pressure, which grows with friction and with the radius-to-height ratio. Multiply by the contact area for the force. The lab shows every step so you can check your hand calculation.
Lab 1 check quiz
References and credits
- S. Kalpakjian and S. R. Schmid, Manufacturing Processes for Engineering Materials, 7th ed., Pearson. Chapter 2 (tension test, true stress and strain, the power law and strain-rate effects) and Chapter 6, Section 6.2 (forging, slab analysis of upsetting). The reference-material K and n values are typical values from Table 2.2 of this book.
- J. H. Hollomon, “Tensile deformation,” Transactions of the AIME, vol. 162, 1945: the power law σ = Kεⁿ.
- A. Considère, Annales des Ponts et Chaussées, 1885: the condition for the onset of necking, dσ/dε = σ.
Lab written by Prof. Olu Emmanuel Femi for MScE6106 Material Manufacturing, Faculty of Materials Science and Engineering, Jimma Institute of Technology. The models follow the sources above, which are credited for them. The text, graphics, example numbers, generated data and quiz on this page are original. They are not taken from the textbook, and this page is not affiliated with or endorsed by its authors or publisher. Students should use their own copy of the textbook.