Friction between the dies and the work stops the metal sliding outwards, so the pressure builds towards the centre. Choose a bar pressed in plane strain or a cylinder upset between flat dies, set the friction and the final height, and see the pressure distribution, the average pressure and the force. Then size a press for an impression-die forging.
- True strain
- –
- Flow stress
- –
- Avg pressure
- –
- Force
- –
Pressure across the die face, from the centre to the free edge, as a multiple of the flow stress. Solid: the slab-method hill, which rises exponentially from the edge and becomes linear where the friction would exceed the shear strength (sticking). Dashed: the linear form behind the average-pressure formula used in the lecture. Dotted: the sticking limit 1/(2μ).
Force against height as the die closes, from the same formula. The horizontal line is the press capacity; the dot is the final height you set.
Size the press for an impression-die forging
F = Kp σf A, with A the projected area including the flash. Kp is an empirical factor for the shape.
- Flow stress
- –
- Force, low Kp
- –
- Force, high Kp
- –
- Press to buy
- –
The bar is the force range from the Kp range. Ticks are standard press sizes (tonnes). Choose the smallest press above the top of the range, because flash thickness, die temperature and billet temperature vary from part to part and an overloaded mechanical press can stall at bottom dead centre.
A good forging fills the die, puts the grain flow along the part and leaves no folds. Close a flash die and watch the cavity fill and the flash form, compare the grain flow in a forged, a machined and a cast part, then diagnose sectioned forgings.
Close the die
- die steel
- hot workpiece
- parting line
Schematic forging load against stroke. Stage 1: the billet upsets and starts to fill the cavity. Stage 2: the cavity is nearly full and flash starts to form. Stage 3: the flash thins and cools in the land, its resistance to flow rises steeply and the pressure fills the last corners.
| Die feature | What it does |
|---|---|
| Parting line | Where the two die halves meet; place it so the part can come out. |
| Land | A narrow, thin gap at the cavity edge. Its cold, thin flash resists flow and builds pressure in the cavity. |
| Gutter | A deeper recess outside the land that holds the excess metal, so the dies can close fully. |
| Draft | A slight taper on the cavity walls (often a few degrees outside, more inside) so the part can be released. |
| Fillets and corner radii | Generous radii help the metal flow and avoid laps and die cracking. |
Grain flow: forged, machined or cast?
The same flanged shaft, sectioned and macro-etched (generated pictures, schematic). Forging bends the flow lines (the stretched inclusions and segregation of the bar) round the shoulder. Machining from a large bar cuts across them and leaves end grains on the surface. A casting has no flow lines at all.
End grains are where flow lines meet a surface. They corrode and start fatigue cracks more easily, which is why crankshafts, connecting rods and hooks are forged so that the flow lines follow the outline.
Diagnose the forging
Each picture is a schematic etched section of a forging with a defect. Read the context, then choose the cause.
The rolls can only pull the strip in if friction is large enough, and the same friction raises the force. Check the bite, find the neutral point, and get the roll force, torque and power for cold or hot rolling. Then plan the passes to reach a target thickness.
- Contact length L
- –
- Flow stress Ȳ'
- –
- Roll force
- –
- Power, both rolls
- –
- Torque per roll
- –
- Strain rate
- –
- Neutral point
- –
- Forward slip
- –
The roll gap, not to scale (the bite is enlarged so you can see it). Marker lines are carried by the strip: they enter slower than the roll surface and leave faster. N is the neutral point, where strip and roll move at the same speed.
Roll pressure along the contact arc from entry to exit, as a multiple of Ȳ' (slab analysis, no front or back tension). The peak is at the neutral point. The dashed line is the average used in the force formula, 1 + μL/2h_av.
Plan the passes
Cold rolling only. Each pass takes the largest bite that the rolls can grip (μ²R) and that the mill can push (force limit). The metal work hardens pass by pass unless it is annealed.
Roll force in each pass against the mill limit (dashed).
Rolling changes the grains as well as the shape. Roll a coarse cast slab hot and watch it recrystallise to fine grains, or roll it cold and watch the grains stretch. Then bend the rolls and see why strip comes out with wavy edges or a buckled centre, and match rolling defects to their causes.
- Passes
- 0
- Total reduction
- 0%
- Grain size
- –
- Grain aspect
- –
Generated micrograph of a longitudinal section (rolling direction left to right, thickness up and down). The magnification changes with the grain size; read the scale bar. Recrystallised grain size from an illustrative empirical relation of the kind used for C–Mn steels, d ≈ 0.5 d₀^0.67 / ε (µm), with a floor of 10 µm.
Roll bending and crown
Bending is greatly exaggerated. A real crown is a fraction of a millimetre on the diameter, and the roll also flattens elastically at the contact, which lengthens the arc and raises the force.
Top: looking along the rolling direction, the two work rolls and the strip between them. Bottom: the strip seen from above after it leaves the mill. Where the strip is thinned more, it is also lengthened more; the shorter parts hold it in tension and the longer parts buckle.
Residual stresses and rolling defects
Lab 3 check quiz
References and credits
- S. Kalpakjian and S. R. Schmid, Manufacturing Processes for Engineering Materials, 7th ed., Pearson. Chapter 6: forging (6.2: slab method, impression-die forging and the Kp ranges, forgeability, defects, die design) and rolling (6.3: roll gap, neutral point, maximum draft, roll force, torque and power, mills, defects and residual stresses).
- E. Siebel, “Die Formgebung im bildsamen Zustande,” 1923, and T. von Kármán, “Beitrag zur Theorie des Walzvorganges,” ZAMM, vol. 5, 1925: the slab (elementary) method for forging and rolling.
- D. R. Bland and H. Ford, “The calculation of roll force and torque in cold strip rolling with tensions,” Proc. Inst. Mech. Eng., vol. 159, 1948: the pressure distribution along the roll arc.
- C. M. Sellars and J. A. Whiteman, “Recrystallization and grain growth in hot rolling,” Metal Science, vol. 13, 1979: the form of the recrystallised grain-size relation used, with illustrative constants.
Lab written by Prof. Olu Emmanuel Femi for MScE6106 Material Manufacturing, Faculty of Materials Science and Engineering, Jimma Institute of Technology. The models follow the sources above, which are credited for them. The text, drawings, generated micrographs, example numbers and quiz on this page are original. They are not taken from the textbook, and this page is not affiliated with or endorsed by its authors or publisher. Students should use their own copy of the textbook.